The metallurgy of iron meteorites
Iron meteorites are pieces of asteroid cores that cooled over millions of years. Their crystal structures and nickel distributions record cooling rates and the size of the bodies they came from.
- Describe the body-centred and face-centred cubic structures of kamacite and taenite.
- Explain the growth of the Widmanstätten pattern using the Fe–Ni phase diagram.
- Explain how metallographic cooling rates are measured and interpreted.
Links to: A-level chemistry: metallic bonding and alloys; A-level geology: crystallisation and cooling rates. The bcc and fcc structures and diffusion modelling go beyond A-level.
Two structures
Iron–nickel alloys adopt two structures. Taenite is face-centred cubic (fcc) and can hold a lot of nickel. Kamacite is body-centred cubic (bcc) and holds at most about 7% nickel. At high temperature, metal with typical meteoritic compositions of 6 to 12% nickel is entirely taenite.
As it cools below roughly 700 to 900 °C, depending on composition, kamacite becomes stable. It nucleates as plates along the octahedral {111} planes of the parent taenite crystal and grows as nickel diffuses out of it into the surrounding taenite.
Widmanstätten patterns
The result, seen on an etched surface, is the Widmanstätten pattern: intersecting kamacite plates in up to four orientations, separated by thin taenite lamellae and fine-grained mixtures called plessite. The width of the kamacite bands is used to classify the meteorites, from coarse to fine octahedrites. Metal with less than about 6% nickel becomes almost entirely kamacite (a hexahedrite); metal with more than about 16% nickel develops only microscopic kamacite (an ataxite).
Diffusion of nickel in iron is very slow at these temperatures. Patterns millimetres wide could only grow over millions of years.
Cooling rates and core sizes
As kamacite grows, nickel piles up at the edges of the taenite, producing M-shaped nickel profiles across taenite lamellae. Measuring these profiles with an electron microprobe and comparing them with diffusion models gives the metallographic cooling rate, typically from a few to thousands of degrees per million years.
If a group of irons all came from one slowly cooling core surrounded by an insulating mantle, they should share one cooling rate. Some groups, such as the IVA irons, show a wide spread, suggesting they cooled in a metal body whose rocky mantle had been stripped away by an impact.
How long to cool?
An iron meteorite has a metallographic cooling rate of 50 °C per million years through the range in which the Widmanstätten pattern grew, from 700 °C to 400 °C. How long did this take?
- Temperature change = 700 − 400 = 300 °C.
- Time = temperature change ÷ cooling rate = 300 ÷ 50.
- Time = 6 million years.
Answer: About 6 million years. Cooling this slow requires a large, well-insulated body, kilometres to tens of kilometres beneath the surface.
Sketch unit cells of bcc and fcc structures and count the atoms per unit cell (2 and 4). Then draw a schematic M-shaped nickel profile across a taenite lamella between two kamacite plates and explain how its shape arises from slow diffusion of nickel.
Print a worksheet A4, with a separate answer sheet for teachers
Quiz
15 questions, picked at random from a bank of 30, so every try is different. Score 12 or more to pass. Choose an answer to see whether you are right and why.
-
Question 1What is the crystal structure of kamacite?
Kamacite is bcc iron–nickel with low nickel; taenite is fcc.
-
Question 2Along which planes of taenite do kamacite plates grow?
Kamacite nucleates along the {111} planes, giving the octahedral geometry of the pattern.
-
Question 3Why do Widmanstätten patterns require slow cooling?
Growth of millimetre-scale kamacite plates needs nickel to diffuse over long distances, which takes millions of years.
-
Question 4What is an ataxite?
With more than about 16% Ni, kamacite forms only microscopically, as in the Hoba meteorite.
-
Question 5What does a wide range of cooling rates within one iron group suggest?
In a mantled core, all parts cool together at one rate; a spread implies an exposed metal body.
-
Question 6Which describes taenite?
Taenite is the fcc iron–nickel phase and can dissolve much more nickel than kamacite.
-
Question 7Why does a body-centred cubic unit cell contain two atoms?
Each corner atom is shared by eight cells: 8 × ⅛ = 1, plus the whole atom at the centre makes 2.
-
Question 8How many atoms belong to one face-centred cubic unit cell?
8 corners × ⅛ = 1, plus 6 face atoms × ½ = 3, giving 4. Counting every atom drawn gives 14.
-
Question 9Metal with 9% nickel is held at about 1,000 °C. What structure does it have?
At high temperature metal with 6 to 12% nickel is wholly taenite; kamacite becomes stable only below roughly 700 to 900 °C.
-
Question 10Why does kamacite appear at different temperatures in different iron meteorites?
Kamacite becomes stable somewhere between about 700 and 900 °C, depending on the metal's composition.
-
Question 11Why must nickel diffuse out of growing kamacite into the surrounding taenite?
The parent taenite has more nickel than kamacite can hold, so the excess must move into the taenite.
-
Question 12Why can a Widmanstätten pattern show kamacite plates in up to four orientations?
Plates grow along the octahedral {111} planes of taenite, and an octahedron has four pairs of parallel faces.
-
Question 13How are the octahedrites subdivided, from coarse to fine?
The width of the kamacite bands is used to classify octahedrites from coarse to fine.
-
Question 14What is plessite?
Plessite is the fine intergrowth that fills spaces between kamacite plates and taenite lamellae.
-
Question 15An iron with 5% nickel cools slowly from its core. What does it become?
Metal with less than about 6% nickel converts almost entirely to kamacite.
-
Question 16A slowly cooled iron with 8% nickel is cut and etched. What would you expect to see?
Between about 6% and 16% nickel, kamacite grows as plates in taenite, giving an octahedrite.
-
Question 17An iron with 18% nickel cooled just as slowly as an octahedrite. Why does it show no visible pattern?
Above about 16% nickel, kamacite develops only on a microscopic scale, giving an ataxite.
-
Question 18Why is a hexahedrite's lack of a Widmanstätten pattern not a sign of fast cooling?
Below about 6% nickel the metal becomes almost entirely kamacite, so there is no taenite to outline plates.
-
Question 19Two irons have the same nickel content, but one has much wider kamacite bands. Which cooled more slowly?
Slower cooling gives nickel more time to diffuse, so kamacite plates grow wider.
-
Question 20Why can't a laboratory reproduce a millimetre-scale Widmanstätten pattern by cooling a melt?
At these temperatures nickel diffusion is so slow that millimetre-wide plates need millions of years.
-
Question 21Why does kamacite growth effectively stop as an iron cools to low temperatures?
Diffusion slows sharply as temperature falls, so the structure is frozen in place.
-
Question 22Across a taenite lamella between two kamacite plates, where is the nickel content highest?
Nickel rejected by growing kamacite piles up at the taenite edges, giving an M-shaped profile.
-
Question 23Why does the nickel profile across a taenite lamella take an M shape?
Slow diffusion within taenite cannot carry the rejected nickel to the centre, so the edges stay nickel-rich.
-
Question 24How are metallographic cooling rates obtained?
Measured M-shaped nickel profiles are matched to models of diffusion at different cooling rates.
-
Question 25An iron cooled at 25 °C per million years from 700 °C to 400 °C. How long did this take?
Time = 300 °C ÷ 25 °C per Myr = 12 Myr.
-
Question 26An iron took 3.0 million years to cool from 700 °C to 400 °C. What was its cooling rate?
Rate = temperature change ÷ time = 300 ÷ 3.0 = 100 °C per million years.
-
Question 27What is a cooling rate of 1,000 °C per million years in degrees per year?
1,000 °C ÷ 1,000,000 years = 0.001 °C per year.
-
Question 28Which is a typical metallographic cooling rate for an iron meteorite?
Measured rates run from a few to thousands of degrees per million years.
-
Question 29Why does a cooling rate of a few degrees per million years imply a large parent body?
Slow cooling needs a well-insulated core, kilometres to tens of kilometres below the surface.
-
Question 30Why would a metal body whose rocky mantle had been stripped away give irons with many cooling rates?
Without insulation, metal near the surface lost heat quickly while deeper metal cooled slowly, as seen in the IVA irons.