Minerals: Advanced course · Lesson 3 of 6

The Fe–Ni system and metallographic cooling rates

The Widmanstätten pattern is a solid-state transformation frozen part-way. Read quantitatively, the widths and nickel profiles of its plates give the cooling rates of asteroid cores, and its finest structures record their magnetic fields.

In this lesson you will
  • Use the Fe–Ni phase relations to explain the nucleation and growth of kamacite from taenite.
  • Explain how nickel diffusion produces M-shaped profiles and how they yield metallographic cooling rates, using square-root scaling of diffusion distance.
  • Describe the low-temperature structures of meteoritic metal: tetrataenite, the cloudy zone, martensite and Neumann bands.

Links to: A-level chemistry: crystal structures of metals and transition metals; A-level physics: thermal physics and magnetism; A-level geology: phase diagrams; A-level maths: square-root and proportional reasoning.

Phase relations

Iron-nickel alloys with meteoritic compositions are single-phase taenite (γ, face-centred cubic) at high temperature. On cooling they enter a two-phase field where kamacite (α, body-centred cubic, low nickel) and taenite coexist, at a temperature that falls with bulk nickel: very roughly 700 °C or more for typical octahedrite compositions of about 7 to 10 wt% Ni. Within the field, the equilibrium compositions diverge as temperature falls: kamacite can hold at most about 7 wt% Ni, while the equilibrium nickel content of taenite rises steeply.

Nucleating kamacite in taenite is difficult. Phosphorus matters: experiments and observations suggest that in many irons kamacite nucleated with, or after, phosphides such as schreibersite, and that phosphorus-poor metal can be undercooled substantially before kamacite appears. The temperature of nucleation sets how long the plates have to grow.

Growth by diffusion

Kamacite grows as plates parallel to the {111} planes of the parent taenite, the four sets of octahedral planes, with a definite crystallographic relationship between the two lattices. As each plate thickens, it rejects nickel into the adjacent taenite. Nickel diffuses quickly in body-centred kamacite but slowly in close-packed taenite, so nickel piles up at the taenite edges. A traverse across a taenite lamella therefore shows an M-shaped profile: high nickel at both rims and a lower central value.

Diffusion coefficients fall exponentially with temperature, and growth effectively stops below roughly 400 °C. A characteristic diffusion distance scales as √(Dt), so a hundred times longer cooling interval gives only about ten times more diffusion. This is why kamacite bandwidths vary over a modest range while cooling rates vary over orders of magnitude.

Metallographic cooling rates

Because the profile depends on how long diffusion ran, the shape of taenite profiles records cooling rate. The classic method compares a lamella's central nickel content with its half-width: for a given half-width, slower cooling allows more nickel to diffuse into the centre, raising the central value. Modern work fits measured profiles with numerical diffusion models that include the phase diagram, nucleation temperature and phosphorus.

Rates range from below 1 °C to many thousands of °C per million years. Within some groups the results are revealing. The IVA irons show cooling rates that vary by more than an order of magnitude and correlate inversely with bulk nickel: the low-nickel metal, which crystallised first, cooled fastest. That pattern fits a metallic body whose insulating mantle had been removed by a collision and which crystallised from the outside inwards, so the first metal to solidify lay near the cold surface, rather than a core buried beneath intact rock.

Low-temperature structures

Below about 400 °C diffusion is too slow for kamacite growth, but new structures still form. Near the rims of taenite, below about 320 °C, nickel and iron atoms order into tetrataenite, FeNi with alternating layers of each, a magnetically hard phase. Further in, the taenite decomposes into the cloudy zone, nanometre islands of tetrataenite in a nickel-poorer matrix. Island size grows as cooling slows, so it gives a second cooling-rate estimate at about 300 °C, and because the islands' magnetisation was set as they formed, the cloudy zone can record a magnetic field present at that time, evidence used to argue for liquid-core dynamos in some parent bodies.

In faster-cooled or reheated metal, taenite transforms without diffusion to martensite. Shock deforms kamacite into thin mechanical twins, Neumann bands, which are especially prominent in hexahedrites.

Worked example

Scaling diffusion distance with cooling rate

Two octahedrites with the same bulk nickel content grew kamacite between the same nucleation temperature and 400 °C, a span of 300 °C. Iron A cooled at 2 °C per million years and iron B at 200 °C per million years. Calculate the growth time for each and estimate how the characteristic diffusion distances compare, assuming √(Dt) scaling with the same effective D.

  1. Growth time A = 300 ÷ 2 = 150 million years; growth time B = 300 ÷ 200 = 1.5 million years.
  2. Ratio of times = 150 ÷ 1.5 = 100.
  3. Diffusion distance ∝ √t, so the ratio of distances = √100 = 10.

Answer: A grew for 150 million years and B for 1.5 million years. A's characteristic diffusion distance is about 10 times B's, so A should have wider kamacite bands and taenite with higher central nickel for a given half-width. Real cooling is not at constant D, because D falls steeply with temperature, so detailed models are used in practice.

Activity

Sketch the M-shaped nickel profile across a taenite lamella between two kamacite plates, labelling the kamacite composition, the rim maximum and the central value. On the same axes, sketch the profile you would expect for a much slower cooling rate with the same half-width. Then write a short explanation of why the IVA cooling rates argue against a core insulated by an intact mantle.

Quiz

15 questions, picked at random from a bank of 30, so every try is different. Score 12 or more to pass. Choose an answer to see whether you are right and why.

  1. Question 1What are the crystal structures of kamacite and taenite?

  2. Question 2How does the temperature of entering the two-phase field change with bulk nickel?

  3. Question 3Within the two-phase field, how does equilibrium taenite composition change on cooling?

  4. Question 4What role does phosphorus appear to play in many irons?

  5. Question 5Why does the nucleation temperature of kamacite matter for bandwidth?

  6. Question 6Phosphorus-poor metal may be undercooled before kamacite appears. What effect does this have?

  7. Question 7Parallel to which planes of taenite do kamacite plates grow?

  8. Question 8Why does nickel pile up at taenite rims?

  9. Question 9What is the shape of a nickel profile across a taenite lamella?

  10. Question 10In which phase does nickel diffuse faster?

  11. Question 11Below roughly which temperature does kamacite growth effectively stop?

  12. Question 12If an iron cooled 10,000 times more slowly, by about how much would the diffusion distance grow?

  13. Question 13Why do bandwidths vary only modestly while cooling rates span orders of magnitude?

  14. Question 14For a given taenite half-width, how does slower cooling affect the central nickel content?

  15. Question 15What do modern cooling-rate methods fit to measured profiles?

  16. Question 16What is the range of metallographic cooling rates?

  17. Question 17In IVA irons, how does cooling rate correlate with bulk nickel?

  18. Question 18Why does the IVA pattern suggest the mantle had been removed?

  19. Question 19Under an intact insulating mantle, what would you expect of cooling rates across a core?

  20. Question 20What is tetrataenite?

  21. Question 21Below about what temperature does tetrataenite form?

  22. Question 22What is the cloudy zone?

  23. Question 23How does cloudy-zone island size relate to cooling rate?

  24. Question 24Why can the cloudy zone record ancient magnetic fields?

  25. Question 25What is martensite in meteoritic metal?

  26. Question 26What are Neumann bands?

  27. Question 27In the worked example, what is iron A's growth time?

  28. Question 28Using √t scaling, two irons' growth times differ by a factor of 25. How do their diffusion distances compare?

  29. Question 29Why is constant-D scaling only an approximation?

  30. Question 30An iron has unusually narrow bands for its nickel and is very phosphorus-poor. Which explanation fits best?